Professional Documents
Culture Documents
Inconel X750 is suitable for use in the high temperature structural operations for gas turbines,
aerospace engines, nuclear power plants, heat processing, formation apparatus and extrusion dies.
Nickel alloy X750 offers extreme resistance to chemical corrosion and oxidation. It has good stress
rupture strength and offers service up to 1500oF or 816oC.
Chemical Composition
Carbon (C)
0.08 %
Manganese (Mn)
0.30 %
Silicon (Si)
0.50 %
Sulfur (S)
0.01 %
Nickel +Cobalt
70 %
Chromium (Cr)
14 to 17 %
Iron (Fe)
5 to 9 %
Aluminum (Al)
0.40 to 1 %
Titanium (Ti)
2.25 to 2.70 %
Copper (Cu)
0.50 %
Columbium + Tantalum
0.70 to 1.20 %
Physical Properties
Density
Melting Point
Co-Efficient of Thermal Expansion
Modulus of Rigidity
Modulus of elasticity
Electric Resistivity
Condition
Hot rolled
Solution Treated
Solution Treated + aged
ohm-cir mil/ft
764
716
746
microhm-mm
1270
1190
1240
Thermal Properties
Temperature
oF
oC
300 oF
149 oC
600 oF
316 oC
1000 oF 538 oC
1200 oF 649 oC
1400 oF 760 oC
1600 oF 871 oC
Thermal conductivity
W/m-K
16.9
20.5
26.5
28.7
31.4
35.3
Modulus of Elasticity
Temperature
oF
oC
80 oF
26.7 oC
500 oF
260 oC
1000 oF
538 oC
1350 oF
732 oC
1500 oF
816 oC
x 10(6) Psi
x 10(6) MPa
31 x 10(6) Psi
28.7 x 10(6) Psi
25 x 10(6) Psi
21 x 10(6) Psi
18.5 x 10(6) Psi
oC
26.7oC to 93oC
26.7oC to 316oC
26.7oC to 538oC
26.7oC to 649oC
10 (-6)/oF
6.7
7.5
7.9
8.1
9
10(-6)/C
12.1
13.5
14.2
14.6
16.2
Thermal Properties
Temp, oF
-250 oF
-200 oF
-100 oF
70 oF
200 oF
Mean Linear
Expansion
6.5
6.6
6.7
7.0
Thermal Conductivity,
Btu/in./hr/sq ft/F
67
70
74
83
89
Specific Heat,
Btu/lb/F
0.073
0.080
0.090
0.103
0.109
Diffusivity,
sq ft/hr
0.150
0.143
0.135
0.132
0.133
Electrical Resistivity,
ohm/circ mil/ft
731
739
Mechanical Properties
Annealed Inconel X750
Temperature, oF
Room temp.
900 oF
1000 oF
1200 oF
Elongation, %
51 %
55 %
55 %
23 %
Tensile strength,
psi
Hot finished + 1300oF for 20 hours air cooled
170,000 psi to
206,000 psi
Hot-finished + Annealed 1800F/1 hr, A.C + 1350F/ 162,000 psi 8 hr, F.C. 100F/hr to 1150F (total 18 hr), A.C
193,000 psi
Hot-finished + 1625F/24 hr, A.C + 1300F/20 hr,
160,000 psi A.C.
188,000 psi
Cold-rolled, annealed +
160,000 psi 1300F/20 hr, A.C.
197,000 psi
Yield
strength, psi
120,000 psi 163,000 psi
115,000 psi 142,000 psi
100,000 psi 135,000 psi
105,000 psi 150,000 psi
Elongation in
2 inch, psi
25 to 15 %
Hardness,
Brinell
313 to 400
30 to 15 %
300 to 390
30 to 15
302 to 363
30 to 20
300 to 400
70 oF
1000 oF
1200 oF
1400 oF
1500 oF
21.1 oC
538 oC
649 oC
760 oC
816 oC
%
Elongation
in 2 inch
22 %
20 %
10 %
10 %
20 %
%
Reduction
of Area
30 %
30 %
21 %
22 %
32 %
Corrosion Resistance
Inconel X750 has corrosion resistance properties similar to Inconel alloy 600. It offers good
resistance to stress corrosion cracking and oxidizing media.
Avaialble Forms
Wire, wiremesh, strip, foil, plate, sheet, rod, bar