You are on page 1of 8

抚顺隆基电磁科技有限公司 实验室

目 录

送 样 单 位:菲律宾铁砂矿-ESM 公司
试 验 员:唐琦
化 验 员:吴威 常荣美
审 核:王珏
报 告 编 写:杨艳萍
试验报告编号:6715-1223
试 验 日 期: 2016 年 12 月 23 日
沈阳隆基电磁科技股份有限公司 实验室
I、Property of Samples:
1.1、Physical character of Samples:
1# is sample from Philippines for the test. 5 small packages of 20kg , gray, 60mesh.
2# is sample from Philippines for the test. 6 small packages of 20kg , gray, 27.6% under 200mesh.

Pic refers to following:

1#package 1#sample

2#package 2#sample
Pic.1:Pictures of sample

2
1.2、Chemical analysis

Table 1:
Item TFe% mFe%
1# sample 38.98 28.63
2# sample 58.16 47.95

1.3、Size of raw material


1#sample sizing refers to Table 2:

Table 2:
Weight Recovery% Fe distribution%
Size/Mesh TFe %
Individual Accumulated Individual Accumulated
+80 5.4 100 11.02 1.53 100
-80+120 33.2 94.6 25.79 21.97 98.47
-120+160 50.5 61.4 47.11 61.03 76.51
-160 10.9 10.9 55.33 15.47 15.47
Total 100 38.98 100

2#sample sizing refers to Table 3.

Table3:
Weight Recovery% Fe distribution%
Size/Mesh TFe %
Individual Accumulated Individual Accumulated
+100 17.2 100 48.67 14.39 100
-100+120 10 82.8 58.24 10.01 85.61
-120+160 39.3 72.8 60.11 40.62 75.59
-160+200 5.9 33.5 61.67 6.26 34.98
-200 27.6 27.6 60.53 28.72 28.72
Total 100 58.16 100

3
II、1# sample magnetic separation testing:
2.1、Relationship of first stage magnetic intensity and separation result.

Table 4:
Magnetic Recovery Yield
Item name TFe% mFe%
Intensity rate % rate %
Feeding 38.98 100 100 28.63
A14 Concentrate 55.35 89.78 63.23 45.01
tailing 10.83 10.22 36.77 0.47
Feeding 38.98 100 100 28.63
A12 Concentrate 56.68 89.05 61.24 46.34
tailing 11.02 10.95 38.76 0.66
Feeding 38.98 100 100 28.63
A9 Concentrate 57.18 88.34 60.22 46.84
tailing 11.43 11.66 39.78 1.07
Feeding 38.98 100 100 28.63
A7 Concentrate 57.32 87.44 59.46 46.98
tailing 12.08 12.56 40.54 1.72

4
2.2、Relationship of second stage magnetic intensity and separation result
Concentrate of first stage (A12) is collected and separated by second stage
magnetic separation

Table 5:
Magnetic
Item name TFe% Recovery rate % Yield rate %
Intensity
Feeding 56.68 100 100
A9 Concentrate 59.25 98.11 93.85
tailing 17.43 1.89 6.15
Feeding 56.68 100 100
A8 Concentrate 59.76 97.72 92.68
tailing 17.66 2.28 7.32
Feeding 56.68 100 100
A7 Concentrate 60.09 97.39 91.87
tailing 18.16 2.61 8.13
Feeding 56.68 100 100
A6 Concentrate 60.17 97.24 91.60
tailing 18.63 2.76 8.40

5
2.3、Relationship of third stage magnetic intensity and separation result
Concentrate of second stage(A7) is collected and separated by third stage magnetic
separation

Table 6:

Gauss strength Item name TFe% Recovery rate % Yield rate %


Feeding 60.09 100 100
A7 Concentrate 61.77 98.02 95.36
tailing 25.58 1.98 4.64
Feeding 60.09 100 100
A4 Concentrate 62.00 97.61 94.61
tailing 26.58 2.39 5.39
Feeding 60.09 100 100
A2 Concentrate 62.18 97.36 94.09
tailing 26.83 2.64 5.91
Feeding 60.09 100 100
A1 Concentrate 62.35 97.08 93.56
tailing 27.25 2.92 6.44

6
2.4、whole magnetic separation flow chart:

Table 7:

Test result of whole magnetic separation

Yield rate % TFe Recovery%


Process stage Item name TFe %
To To raw To To raw
feeding material feeding material

First stage feeding 100 38.98 100


magnetic separation concentrate 61.24 56.68 89.05
A12 tailing 38.76 11.02 10.95

Second stage feeding 100 61.24 56.68 100 89.05


magnetic separation concentrate 91.87 56.26 60.09 97.39 86.73
A7 tailing 8.13 4.98 18.16 2.61 2.32

Third stage feeding 100 56.26 60.09 100 86.73


magnetic separation concentrate 94.09 52.94 62.18 97.36 84.44
A2 tailing 5.91 3.32 26.83 2.64 2.29

2.5、work flow sketch

Philippines iron sand 1# sample work flow sketch

7
III、Conclusion:
3.1、 The iron sand sample is provided from Philippines. Testing is about 1#sample.
3.2、 1# sample is tested by first stage(A12)+second stage(A7) +third stage (A2)
magnetic separation
Table8:

Concentrate
Item Yield TFe TFe% Tailing
TFe%
rate% Recovery%

1# Sample 52.94 62.18 84.44 12.89


3.3、The testing is only responsible for the iron sand sent to the lab.

LONGI MAGNET CO LTD

DEC.23,2016